The contact method is a variant of tip ignition. The stud rests on the workpiece with its ignition tip before welding. Here you can find out how the process works and what it is suitable for.
In short
In the contact method, the stud is preloaded against the workpiece by a spring force. When welding is triggered, the ignition tip melts instantly, the arc ignites and the spring presses the stud into the molten pool. Thanks to the higher joining force and longer welding time, the method is particularly suitable for steel, stainless steel and galvanised sheet.

On this page
How does the contact method work?
In contact welding, the stud is preloaded against a spring force when the welding gun or automatic welding head is placed on the workpiece. This means that electrical contact between the ignition tip of the stud and the workpiece exists right from the start.
When the operator or the automation triggers the weld, the ignition tip melts instantly and ignites the arc between the stud flange and the workpiece.
The spring force then moves the stud towards the workpiece by the distance freed up by the melting of the ignition tip. Once the stud has finally been placed, the molten pool solidifies.
What is the timing of a weld?
The graphic above shows the typical sequence in four steps:
- 0 ms, placing: The stud rests on the workpiece with its ignition tip under spring force.
- 1 ms, ignition: The ignition tip melts and the arc ignites.
- 1.5 ms, plunging: The spring presses the stud into the molten pool.
- 2 ms, solidification: The molten pool solidifies and the joint is complete.
Which materials is the contact method suitable for?
Suitable materials are steel, stainless steel, aluminium, brass and metal-coated sheet. Thanks to the higher joining force and longer welding time, the contact method is particularly suitable for steel and stainless steel as well as for galvanised sheet.
How does it differ from the gap method?
In the contact method, the stud rests on the sheet with its ignition tip before welding. In the gap method, it is held at a small distance and only placed on the sheet during welding. The gap method has a shorter welding time and a lower joining force and is therefore mainly used for aluminium and in automation.
What technical data apply?
| Parameter | Value |
|---|---|
| Stud diameter d (mm) | 0.8 to 8 (aluminium up to 6) |
| Welding time approx. (ms) | 1-4 |
| Spring force approx. (N) | 60-100 (depending on piston dimensions and bearing) |
| Impact speed approx. (m/s) | 0.5-0.7 |
| Min. workpiece thickness (mm) | 0.5 |
You can find all parameters compared with the gap method on the tip ignition page. Values may vary depending on unit and application.
Would you like to know whether the contact method suits your component?
We will be happy to advise you personally, by phone on +49 2302 95640-0 or by message.
More topics
Strengths, applications and key data at a glance.
Short welding time, ideal for aluminium and automation.
Tip ignition or drawn arc? All processes at a glance.
Stainless steel, aluminium, galvanised sheet and more.